管线钢X80卷板横裂纹成因与轧制工艺改进Genesis of transverse cracks in pipeline steel X80 and improvement of rolling process
文新理,蒋波,刘翔,刘雅政
摘要(Abstract):
利用光学显微镜和扫描电镜观察了管线钢X80卷板横裂纹的微观形貌和组织特征,利用Gleeble-3800热模拟试验机测定了X80材料的动态连续冷却转变曲线(动态CCT曲线),在国内某生产线上进行了轧制实验和工艺优化。结果表明:精轧过程先共析铁素体的析出是导致横裂纹的根本原因,进入精轧机组的中间坯厚度(BH)和终轧温度(FDT)对X80卷板的表面质量和力学性能有重要影响,当BH=55 mm、FDT=800℃时表面质量和力学性能均合格。
关键词(KeyWords): 管线钢X80;横裂纹;轧制工艺;表面质量
基金项目(Foundation): 中央高校基本科研业务费专项资金资助(FRF-TP-12-046A);; 北京高校“青年英才计划”
作者(Author): 文新理,蒋波,刘翔,刘雅政
DOI: 10.13289/j.issn.1009-6264.2014.11.017
参考文献(References):
- [1]庄传晶,冯耀荣,李鹤林,等.国内X80级管线钢的发展及今后的研究方向[J].焊管,2005,28(2):10-14.ZHUANG Chuan-jing,FENG Yao-rong,LI He-lin,et al.The development and its Future research direction of grade X80 pipeline steel in China[J].Welded Pipe and Tube,2005,28(2):10-14.
- [2]柳得橹,邵伟然,孙贤文,等.钢的表面带状组织及其引起的冷弯裂纹[J].北京科技大学学报,2005,27(1):40-44.LIU De-lu,SHAO Wei-ran,SUN Xian-wen,et al.Superficial banded structure and its effects on bending flaws of low carbon steel strips[J].Journal of University of Science and Technology Beijing,2005,27(1):40-44.
- [3]张骁勇,高惠临,吉玲康,等.X100管线钢连续冷却转变的显微组织[J].材料热处理学报,2010,31(1):62-66.ZHANG Xiao-yong,GAO Hui-lin,JI Ling-kang,et al.Microstructure of X100 high strength pipeline steel during continuous cooling transformation[J].Transactions of Materials and Heat Treatment,2010,31(1):62-66.
- [4]余伟,谢勇,武会宾,等.X120管线钢的连续冷却相变及显微组织[J].材料热处理学报,2011,32(3):62-66.YU Wei,XIE Yong,WU Hui-bin,et al.Continuous cooling phase transformation and microstructure of X120 pipeline steel[J].Transactions of Materials and Heat Treatment,2011,32(3):62-66.
- [5]沈丙振,周进,韩志强,等.热轧全流程带钢温度场数值模拟[J].清华大学学报:自然科学版,2003,43(5):601-604.SHEN Bing-zhen,ZHOU Jin,HAN Zhi-qiang,et al.Numerical simulation of plate temperature distribution during hot rolling[J].Journal of Tsinghua University:Science and Technology,2003,43(5):601-604.
- [6]王有铭,李曼云,韦光.钢材的控制轧制和控制冷却(第2版)[M].北京:冶金工业出版社,2009:32-35.
- [7]廖波,肖福仁.针状铁素体管线钢组织及强韧化机理研究[J].材料热处理学报,2009,30(2):57-62.LIAO Bo,XIAO Fu-ren.Research on microstructure and strength-toughening mechanism of acicular ferrite pipeline steel[J].Transactions of Materials and Heat Treatment,2009,30(2):57-62.
- [8]KONG De-jun,LONG Dan,WU Yong-zhong,et al.Analysis of impact toughnesss and fracture morphologies of X80 pipeline steel welded joints with submerged-arc welding[J].Journal of Materials Engineering,2013,3(6):50-54.
- [9]Han S Y,Sohn S S,Shin S Y,et al.Effects of microstructure and yield ratio on strain hardening and Bauschinger effect in two API X80 linepipe steels[J].Materials Science and Engineering A,2012,551:192-199.
- [10]Sung H K,Sohn S S,Shin S Y,et al.Effects of finish rolling temperature on inverse fracture occurring during drop weight tear test of API X80 pipeline steels[J].Materials Science and Engineering A,2012,541:181-189.
- [11]崔忠圻.金属学与热处理[M].北京:冶金工业出版社,2000:270-273.
- [12]任毅,张帅,王爽.组织形貌对X80管线钢性能的影响[J].北京科技大学学报,2007,29(8):798-802.REN Yi,ZHANG Shuai,WANG Shuang.Effect of structure pattern on the performance of X80 pipeline steel[J].Journal of University of Science and Technology Beijing,2007,29(8):798-802.
文章评论(Comment):
|
||||||||||||||||||
|
||||||||||||||||||